96.5% High purity DBM 97% High purity DBM 97.5% High purity DBM 98% High purity DBM
Send InquiryChat NowHigh Purity Dead Burned Magnesia
Description
About 70% materials within 200μm under a 15% moisture content will be feed into MHF after drying by the hot exhaust gas from the drier. The calcined MgO can be cooled to<100℃ by water-cooling screw.
The fines will become briquettes after grinding and briquetting. These briquettes are the feeding material for the dead burn by shaft kiln on a temperature of 2,000℃ to create high-purity magnesia.
Picture
![]() | ![]() | ||
96.5% | 97% | 97.5% | 98% |
Specification
Item | MgO% | LOI% | SiO2% | CaO% | Fe2O3% | Al2O3% | B.D.(g/cm3) |
96.5% High purity DBM | 96.47 | 0.17 | 0.67 | 1.47 | 0.62 | 0.1 | 3.35 |
97% High purity DBM | 97.45 | 0.17 | 0.55 | 1.18 | 0.56 | 0.09 | 3.35 |
97.5% High purity DBM | 97.74 | 0.16 | 0.46 | 1.06 | 0.5 | 0.08 | 3.37 |
98% High purity DBM | 98.4 | 0.14 | 0.26 | 0.64 | 0.51 | 0.05 | 3.381 |